dparndt

Mechanical
Feb 24, 2010
5
I have a 440C part that is tempered at 400 F to a Rockwell C hardness of 58-60. I am looking into a coating process that needs to be done at 428 F. Will being at that temperature reduce the hardness or change any of its other properties significantly?
 
Replies continue below

Recommended for you

You should be right ~Rc58 after some time at 428F, according to my old Carpenter SS book. Watch out for decarb.

"You see, wire telegraph is like a very long cat. You pull his tail in New York and his head is meowing in Los Angeles. Do you understand this? Radio operates the same way: You send signals here, they receive them there. The only difference is there is no cat." A. Einstein
 
Hardly. But I've heat treated a lot of 440C, and if the austenitizing furnace atmosphere is the least bit oxidizing or not reducing enough, it will decarb.