Material 12L14 case harden R15N 88-90 case deep 3.81mm
give me process detail and it require to grinding allow
 
Replies continue below

Recommended for you

12L14 material is not suited for that depth of hardening. To achieve a case depth of 3.81mm/0.150" a material with higher alloy content such as 8620 would be needed.
 
If a very deep case is desired it might be worth looking at another approach, such as induction hardening a material like 4340H. You can easily achieve 0.150" case depth with the IH process.
 