I've ran 2 PQR tests on duplex stainless steels.
1 X PQR on 22%Cr duplex UNS S31803 - 76mm OD X 19.1mm THK machined from forged bar
1 X PQR on 25%Cr super duplex UNS S32760 - 76mm OD X 19.1mm THK machined from forged bar
GTAW, 98Ar 2N shield & purge
Both PQRs have failed on tensiles in the parent material at values below the min req in ASME IX. 22Cr - 559MPa. 25Cr - 599MPa
Done tensiles on the parent material and both results are well above the min requirement. 22Cr - 772MPa. 25Cr - 844MPa
impacts, hardness, macro, bends all acceptable on PQR
Has anyone experienced loss of tensile strength in the parent due to weldng of duplex? Or can offer any advise on an explanation for this?
1 X PQR on 22%Cr duplex UNS S31803 - 76mm OD X 19.1mm THK machined from forged bar
1 X PQR on 25%Cr super duplex UNS S32760 - 76mm OD X 19.1mm THK machined from forged bar
GTAW, 98Ar 2N shield & purge
Both PQRs have failed on tensiles in the parent material at values below the min req in ASME IX. 22Cr - 559MPa. 25Cr - 599MPa
Done tensiles on the parent material and both results are well above the min requirement. 22Cr - 772MPa. 25Cr - 844MPa
impacts, hardness, macro, bends all acceptable on PQR
Has anyone experienced loss of tensile strength in the parent due to weldng of duplex? Or can offer any advise on an explanation for this?