What is the major cause of cracking in L-605 alloy?
We have struggled with problem on and off for years and never figured it out.
Thank you
 
Replies continue below

Recommended for you

FWMengineering;
Can you provide some additional background information as to use of this material in service??? What type of cracking???
 
It is in wire form going for straight cut bar.
The major amount of cracking has been of a stress corrosion type making our cleaning suspect.
However we also trying to anneal with a vacuum furnace and the ramp up to temperature is slow
and the quench is on boarder line of being to slow.
Thank you

 
What is the original heat treatment condition for your processing? This is a cobalt-based material and from the literature I have seen when exposed to intermediate temperatures can result in loss of ductility.
 
Recommended 2200F air anneal 1 to 2 hours water quench.
We are trying to use a 2 bar vac furnace with helium argon mix
 