I am still over phosphating parts. I cant give too much detail but I can give this much.
My pre-rinse is at a pH of 5.93 and a temp of 47C
my pre-phosphate is at a pH of 5.23 and a temp of 49.3C
my phosphate is at a pH of 5.13 and temp of 50.7
my cold rinse is at a pH of 5.76 and a temp of 51.5C
my hot rinse is at a pH of 6.3 and a temp of 68.5C
My bottom pressure (for the underside of the part) is set lower than the top.
I dont know the temp of the dryer.
My nozzels are clean and set in the correct position.
My concnetration of phosphate and pre-phoshate is at company standards.
The racks they are laying on have been cleaned.
Im running out of things to check.
Is there anything else I can do to keep my parts from over phospahting.
Should I raise the pH of the rinse tanks or even the phosphate tanks themselves?
Plus, my last question. Could the color of rose gold be from, the parts going through the drying process? Is there a color change that happens to phosphate from going through a dryer?
Thanks so much for your help, It has really helped me out.
cmwatson78
My pre-rinse is at a pH of 5.93 and a temp of 47C
my pre-phosphate is at a pH of 5.23 and a temp of 49.3C
my phosphate is at a pH of 5.13 and temp of 50.7
my cold rinse is at a pH of 5.76 and a temp of 51.5C
my hot rinse is at a pH of 6.3 and a temp of 68.5C
My bottom pressure (for the underside of the part) is set lower than the top.
I dont know the temp of the dryer.
My nozzels are clean and set in the correct position.
My concnetration of phosphate and pre-phoshate is at company standards.
The racks they are laying on have been cleaned.
Im running out of things to check.
Is there anything else I can do to keep my parts from over phospahting.
Should I raise the pH of the rinse tanks or even the phosphate tanks themselves?
Plus, my last question. Could the color of rose gold be from, the parts going through the drying process? Is there a color change that happens to phosphate from going through a dryer?
Thanks so much for your help, It has really helped me out.