One of our suppliers states in his P&P procedure that duplex steel pipes can be treated for a time "up to 24 hours". Solution used is 10%-16% nitric acid + 5%-8% hydrofluoric acid in water at ambient temperature (10-25 °C)
Isn't it a very long dwell time? Is there any risk of damaging the pipe surface? And besides, are there any methods to speed up the process?
Thanks
Max
 
Replies continue below

Recommended for you

This is a pickle, not a passivation.
We pickle warm. 20% nitric + 5% HF at about 125-130F. Only some of the high alloy Ni-Cr-Mo grades take more than 2 hours. 304 usually thakes about 20-30 min.
At low temp you will not get much attack at all.

= = = = = = = = = = = = = = = = = = = =
Rust never sleeps