PQR with two processes

Status
Not open for further replies.

fazel1

Industrial
May 7, 2005
69
we have a 15mm plate for PQR which is welded by two processes: 4mm GTAW and 11mm SMAW . can we write a WPS for a 19mm thickness plate only with SMAW process by support of that PQR?
 
Replies continue below

Recommended for you

Yes, the 19mm is within the maximum qualified SMAW deposit thickness of 22mm per QW-451.
 