2,271
I'm curious if anyone has any experience of what this materials low temperature toughness characteristics are like? How will it perform at -20, 0, 32 °F?
 
Replies continue below

Recommended for you

We have had occasion to test some failed parts. In the K-Zone of the web, absorbed energy values as low as 5 ft-lbs were obtained at 60 F. 20 to approximately 50 ft-lb absorbed energy values were obtained in the web away from the K-Zone at 20 F.

 