Mar 31, 2008 #1 Yoman Mechanical Joined Dec 8, 2005 Messages 9 Location GB The Duplex 25% has SMYS of 448MPa, UTS of 656MPa and Elongation of 25%. If I like to plot the stress Vs strain curve with Ramberg-os'good behaviour. what strain will the UTS be? 25%? Many Thanks
The Duplex 25% has SMYS of 448MPa, UTS of 656MPa and Elongation of 25%. If I like to plot the stress Vs strain curve with Ramberg-os'good behaviour. what strain will the UTS be? 25%? Many Thanks
Mar 31, 2008 #2 CoryPad Materials Joined Apr 15, 2002 Messages 5,192 Location US No, the UTS will be at less than 0.25 strain. It will be at a strain equal to the strain hardening exponent, n. Regards, Cory Please see FAQ731-376 for tips on how to make the best use of Eng-Tips Fora. Upvote 0 Downvote
No, the UTS will be at less than 0.25 strain. It will be at a strain equal to the strain hardening exponent, n. Regards, Cory Please see FAQ731-376 for tips on how to make the best use of Eng-Tips Fora.
Mar 31, 2008 #3 metengr Materials Joined Oct 2, 2003 Messages 15,478 Location US .....where you would need to plot log true stress and log true strain to determine n as CoryPad mentioned. Upvote 0 Downvote
.....where you would need to plot log true stress and log true strain to determine n as CoryPad mentioned.