I am looking for a Fine Pearlite stucture after a piece of rail is thermite welded. The rail steel is essentially a 1080 Carbon Steel. Specifically the composition is:
Weight Percentage, %

Carbon, C
0.72 - 0.84

Manganese, Mn
0.70 – 1.25

Silicon, Si
0.10 – 1.00

Phosphorus, P
0.02 Max.

Sulphur, S
0.02 Max.

Copper, Cu
0.40 Max.

Chromium, Cr
0.20 – 0.40

Nickel, Ni
0.15 Max.

Molybdenum, Mo
0.05 Max.

Vanadium, V
0.01 Max.

Aluminium, Al
0.01 Max.

Based on a CCT Diagram for 1080 steel it should be cooled from Eutectoid temp of 727°C to 25°C no quicker than 2 minutes and no longer than 166 minutes. Does this make sense. See attached.

 
Replies continue below

Recommended for you

Yes, that would be my interpretation of the diagram, but you may want to do some experimenting and lab work for verification. As compared to spec-grade 1080, the chemistry you have listed has boosted levels of Si, Mn, and Cr among others that could affect 'hardenability' and bias the resulting microstructure, probably toward the P+M zone.
 
What I don't get is the 40°C/s and the 5°C/s it doesn't match with the time scale on the x-axis?
 
The time scale on the x-axis is just seconds (s) of time and your comparing a cooling rate of deg C/s to seconds.
 
Yes I understand that, I'm not that slow.

I don't understand a) how is the cooling rate constant?

b)If we take a constant cooling rate of 40C/s, it means that from 730C to 0C, it would take 18.3 seconds. That doesn't match the x-scale which says 10^2.
 
The cooling rates associated with the three curves (5, 40, 140 C/s) are incorrect with respect to the x-axis. The author and editor(s) of this textbook did not catch the error. If you look at other CCT diagrams you can see that a cooling rate of 40 C/s is associated with the 10 second order of magnitude, not 102.
 
Ok so I should cool the steel from the critical temp no quicker than 10 seconds and no longer than 166 minutes?
 