We have been trying to complete a PQR for super duplex pipe. As per client specification this PQR must pass G48-A 40degC. We have passed all other testing requirements, except for the G48.
Pipe: ASTM A790 USN32750
Size: 200NB sch 40 and 200NB sch 20
Position 5G vertical up
backing gas: Ar + 2%N
shielding gas: 100% Ar
process: GTAW
Filler wire: 2.4mm Er2594
We have passed hardness testing, macro and ferrite count good, no sigma phases some surface level martensite detected along with precipitates.
My thoughts from hear are the following:
1. change baking(purge) gas to 100% N
2. change brand of wire from Exton to Bohler Welding – Avesta 2507/P100 GTAW as this is batch tested with G48 testing
could some please help in regards to the Formier gas ( I am not sure if I can get it in my contrary) but if I can is 95%N+5%H better for super duplex will it help much with reducing the heat tint coloring, is there a problem with hydrogen cracking using the gas? Should I use these gas for backing purge?
Thanks very much.
We have been trying to complete a PQR for super duplex pipe. As per client specification this PQR must pass G48-A 40degC. We have passed all other testing requirements, except for the G48.
Pipe: ASTM A790 USN32750
Size: 200NB sch 40 and 200NB sch 20
Position 5G vertical up
backing gas: Ar + 2%N
shielding gas: 100% Ar
process: GTAW
Filler wire: 2.4mm Er2594
We have passed hardness testing, macro and ferrite count good, no sigma phases some surface level martensite detected along with precipitates.
My thoughts from hear are the following:
1. change baking(purge) gas to 100% N
2. change brand of wire from Exton to Bohler Welding – Avesta 2507/P100 GTAW as this is batch tested with G48 testing
could some please help in regards to the Formier gas ( I am not sure if I can get it in my contrary) but if I can is 95%N+5%H better for super duplex will it help much with reducing the heat tint coloring, is there a problem with hydrogen cracking using the gas? Should I use these gas for backing purge?
Thanks very much.