Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations KootK on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

347H vs 347

Status
Not open for further replies.

Eduardo1982

Mechanical
Oct 31, 2014
65
Hey guys.
Does anyone is familiar with 347H Stainless Steel? I have read that this material is highly recommended to work in solar industry (high temperature and working with molten salts). Actually I wish to know why this 347H is recommended instead of 347. Is there any literature that talks about corrosion rates in molten salt baths for such materials?
Any info I will appreciate.
 
Replies continue below

Recommended for you

What flavor of salt? These materials would not be acceptable for chloride salts.
 
TugboatEng
Molten salts are typically made up of 60% sodium nitrate and 40% potassium nitrate.
Working temperatuve range about 350-560 °C.
 
Most of the work that I recall used ferritic SS for this, such as 430.
347H can be tough to work with. Since it has high C it much have higher Nb, and that can welding difficult.

= = = = = = = = = = = = = = = = = = = =
P.E. Metallurgy, consulting work welcomed
 
Eduardo,
Yes, that would be the case at the top end of the temp range.
But at even slightly lower temps the ferritic will be stronger.
And the lower thermal expansion (almost 50%) greatly reduces stresses with thermal cycling.
This is important since these plants cycle from cool to hot every day.
There are also higher C grades of ferritic that may be suitable.
In the past I have supplied 625 for solar absorber tubes (annealed in air and the oxide left on them) and 439 for heat exchangers (sort of steam generators).

= = = = = = = = = = = = = = = = = = = =
P.E. Metallurgy, consulting work welcomed
 