How to compound AEM to withstand DOT 3,4,5 brake fluids?
 
Replies continue below

Recommended for you

Get rid of the acrylic part, and add propylene and some diene monomer. I.e. use EPDM instead.
 
For barke fluid resistance the better product will be EPM or EPDM with low diene contente, cured by peroxide. Compared to AEM the price will be low.
 