Jun 19, 2007 #1 cmn8226 Mechanical Apr 2, 2007 32 0 0 US Hey guys, I have a requirement for SB167 UNS NO6601 (alloy 601) pipe. does all 601 pipe come solution annealed? I am requiring it with a solution annealed HT process, and I am not sure if they come otherwise. thanks
Hey guys, I have a requirement for SB167 UNS NO6601 (alloy 601) pipe. does all 601 pipe come solution annealed? I am requiring it with a solution annealed HT process, and I am not sure if they come otherwise. thanks
Jun 19, 2007 #2 metengr Materials Oct 2, 2003 15,478 0 0 US cmn8226; I reviewed SB 167-01, and this specification provides the following options for N06601; hot-worked annealed cold worked annealed annealed = solution annealed performed at 2100-2250 deg F, and either quenched in water or rapidly cooled. Upvote 0 Downvote
cmn8226; I reviewed SB 167-01, and this specification provides the following options for N06601; hot-worked annealed cold worked annealed annealed = solution annealed performed at 2100-2250 deg F, and either quenched in water or rapidly cooled.
Jun 19, 2007 Thread starter #3 cmn8226 Mechanical Apr 2, 2007 32 0 0 US so when the MTR says annealed, it implies its solution annealed? because thats all it says as far as 'condition' Upvote 0 Downvote
so when the MTR says annealed, it implies its solution annealed? because thats all it says as far as 'condition'
Jun 19, 2007 #4 metengr Materials Oct 2, 2003 15,478 0 0 US If the material was procured in accordance with SB 167, yes. Upvote 0 Downvote