May 29, 2010 #1 Enp12444 Civil/Environmental Nov 30, 2002 5 0 0 EG Hi Guys, I am wondering if you can help me specify a riser clamp neoprene liner that would work effectively in marine environment.
Hi Guys, I am wondering if you can help me specify a riser clamp neoprene liner that would work effectively in marine environment.
May 30, 2010 1 #2 SJones Petroleum Apr 22, 2001 3,890 0 36 GB DNV-RP-F106, Coating Data Sheet No. 7 Steve Jones Materials & Corrosion Engineer http://www.oilandgaspeople.com/cv/11499664http://www.linkedin.com/pub/8/83b/b04 Upvote 0 Downvote
DNV-RP-F106, Coating Data Sheet No. 7 Steve Jones Materials & Corrosion Engineer http://www.oilandgaspeople.com/cv/11499664http://www.linkedin.com/pub/8/83b/b04
May 31, 2010 Thread starter #3 Enp12444 Civil/Environmental Nov 30, 2002 5 0 0 EG Many thanks Steve appreciate it, I checked it out and seems great yet I am still wondering if the same compression set requirements apply to the clamp liners? Any thoughts about the acceptance criteria for seawater absorption & ozone resistance for such application? Upvote 0 Downvote
Many thanks Steve appreciate it, I checked it out and seems great yet I am still wondering if the same compression set requirements apply to the clamp liners? Any thoughts about the acceptance criteria for seawater absorption & ozone resistance for such application?
May 31, 2010 #4 SJones Petroleum Apr 22, 2001 3,890 0 36 GB Seawater absorption: - Max 5% volume change - Reduction in tensile strength max 15% - Change in hardness max +5/-5 units - No cracking, crazing, blistering or splitting after immersion Ozone resistance: - No cracking or 'other detrimental effects' Steve Jones Materials & Corrosion Engineer http://www.oilandgaspeople.com/cv/11499664http://www.linkedin.com/pub/8/83b/b04 Upvote 0 Downvote
Seawater absorption: - Max 5% volume change - Reduction in tensile strength max 15% - Change in hardness max +5/-5 units - No cracking, crazing, blistering or splitting after immersion Ozone resistance: - No cracking or 'other detrimental effects' Steve Jones Materials & Corrosion Engineer http://www.oilandgaspeople.com/cv/11499664http://www.linkedin.com/pub/8/83b/b04
Jun 1, 2010 Thread starter #5 Enp12444 Civil/Environmental Nov 30, 2002 5 0 0 EG Thanks Steve, actualy thanks twice for the two replies much appreciate the expert advice Upvote 0 Downvote