I am attempting to perform several magnetic analyses, but I couldn't find B-H curve for 1018 steel. I have read a former thread posted on 23-Jul-04, but I couldn't find any data with the link mentioned.
Could anyone send me these data? Thank you in advance.
 
Replies continue below

Recommended for you

0.000000 0.00
The following was taken from an FEA magnetic program for 1018 low carbon alloy. It also contains data for highly saturated condition.
B (Tesla) H (amp/m)
0.250300 238.73
0.925000 795.78
1.250000 1591.55
1.390000 2387.33
1.525000 3978.88
1.710000 7957.75
1.870000 15915.50
1.955000 23873.25
2.020000 39788.75
2.110000 79577.50
2.225000 159155.00
2.430000 318310.00

 
Thank you very much for your help.
 
What is the FEA magnetic program, where I can find it ?
 
zacky,

It is better to start a new thread when one has a new/different question.

There is a list of some magnetic modeling software packages in the FAQ section: See faq340-1112
 
Status
Not open for further replies.

Part and Inventory Search

Sponsor