Hi Guys,
I recently noticed that there is significant difference between the predicted life with S/N curves shown in Figures 3.7.5.2.8(b)and 3.7.5.2.8(e) in MMPDS-09. Both of them are "for unnotched 7050-T7451 plate, long transverse direction, t/4 specimen locations". The second one is giving very conservative results comparing to the first one. I would like to know how we can explain this significant difference? I also noticed that these curves are not shown in MMPDS-15.
Thanks,
A.
 
Replies continue below

Recommended for you

Give us the rest of the figure titles, including any footnotes.
These are very detailed.
If in doubt contact Battell Columbus, they maintain MMPDS data.

= = = = = = = = = = = = = = = = = = = =
P.E. Metallurgy, consulting work welcomed
 
Figure 3.7.5.2.8(b):
Product Form = 4.25 to 8.50 inches thick
Specimen Details: Unnotched 0.25 inch diameter
Surface Condition: Polished, final surface finish unspecified
Test Parameters: Loading - Axial, Frequency - 20 Hz, Temperature - RT, Environment - Air
No. of Heat/Lots: Unspecified
Sample Size = 57
Std. Error of Estimate = 0.183
Standard Deviation = 0.814
R^2 = 95%

Figure 3.7.5.2.8(e):
Product Form = 1 to 6 inches thick
Specimen Details: Unnotched 0.25 and 0.30 inch diameter
Surface Condition: Not Specified
Test Parameters: Loading - Axial, Frequency - 800 cpm and unspecified, Temperature - RT, Environment - Air
No. of Heat/Lots: 15
Sample Size = 85
Std. Error of Estimate = 0.507
Standard Deviation = 0.794
R^2 = 59%


 