We are anticipating casting 17-4 PH stainless steel. The castings will weigh 6000-8000 pounds. The wall thicknesses will average about 4-5 inches. The chemistry will be as specified in CB7CU1. Any input from foundrymen knowledgeable with these castings would be appreciated, specifically - do we shake out hot or cold? How do we avoid excessive delta ferrite?
 
Replies continue below

Recommended for you


This is the first one that I found. As I recall you are going to need to modify the chemistry and use some special casting practices.

What properties are you looking for? How do you intend to heat treat this?

= = = = = = = = = = = = = = = = = = = =
Rust never sleeps
Neither should your protection
 
I have cast runner blades this weight in CA6NM. So I do not see any major changes to be incorporated for processing your castings in 17-4 PH alloy.

Use conventional wisdom and adopt sound foundry practices. It will be good if you could give a cold shake out. Heavily chill the thick sections . My main concern will be regarding homogenizing these castings and then cooling it fast.

You could also try casting a small part of equivalent section thickness and then perform various heat tret cycles to get the best properties and microstructure.

 
Heat treatment of the heavy section 17-4PH castings will consist of homogenization at 2100 degrees F, solution at 1900 deg.F, followed by hardening at 1150 deg.F.
 