Dec 18, 2008 #1 sigma38 Aerospace Apr 10, 2007 25 0 0 US For small areas of cad plating that have worn, or been machined, off of steel and nickel-aluminum-bronze (e.g. bushings), what are folks seeing done to protect the surface without having to re-cad plate?
For small areas of cad plating that have worn, or been machined, off of steel and nickel-aluminum-bronze (e.g. bushings), what are folks seeing done to protect the surface without having to re-cad plate?
Dec 18, 2008 #2 MintJulep Mechanical Jun 12, 2003 9,806 1 38 JP Iridite http://galladechem.com/specs/macdermid/78650.pdf Upvote 0 Downvote
Dec 19, 2008 Thread starter #4 sigma38 Aerospace Apr 10, 2007 25 0 0 US Could you tell us more about "brush cadmium plating"? Do you have material and application specification references by chance? Thanks. Upvote 0 Downvote
Could you tell us more about "brush cadmium plating"? Do you have material and application specification references by chance? Thanks.
Dec 19, 2008 Thread starter #5 sigma38 Aerospace Apr 10, 2007 25 0 0 US Actually, let me adjsut the question... a quick google brought up a lot of info... what spec seems to be the aero industry standard for this process? Upvote 0 Downvote
Actually, let me adjsut the question... a quick google brought up a lot of info... what spec seems to be the aero industry standard for this process?
Dec 19, 2008 #6 MintJulep Mechanical Jun 12, 2003 9,806 1 38 JP The Iridite made the US Navy happy for ship-board stuff back in the days when I was building stuff for the Navy. Upvote 0 Downvote
The Iridite made the US Navy happy for ship-board stuff back in the days when I was building stuff for the Navy.
Dec 20, 2008 #7 Flesh Materials Jul 17, 2003 108 0 0 US Standards: AMS 2451/4B --Plating, Brush, Cadmium Corrosion Protective, Low Hydrogen Embrittlement AMS-QQ-P-416 --Plating, Cadmium (Electrodeposited) Upvote 0 Downvote
Standards: AMS 2451/4B --Plating, Brush, Cadmium Corrosion Protective, Low Hydrogen Embrittlement AMS-QQ-P-416 --Plating, Cadmium (Electrodeposited)
Dec 30, 2008 #8 WKTaylor Active member Sep 24, 2001 3,974 0 36 US MIL-STD-865D Selective Brush Plating, Electro-Deposition Regards, Wil Taylor Upvote 0 Downvote