GRoberts
Materials
- Apr 22, 2002
- 548
We have had fairly good luck with the particular brand of E71T-1 FCAW wire we use when testing CVNs at -50F after 1125F PWHT. Recently one of our customers specified an 1175F minimum PWHT temperature. After 1175F, the CVNs did rather poorly at -50F. (We also tested E7018-1 in parallel, and of course it did wonderfully) Anybody have any luck with low temp CVNs using a carbon steel FCAW electrode after 1175F or higher PWHT? We are just welding carbon steel, so most of the non-carbon steel electrodes we have used that would perform well at -50F severly overmatch the base metal with regards to strength, or have more than 1% Ni, and we have to meet NACE.