Electroless Nickel Plating Thickness Limit

Status
Not open for further replies.

Schuyler

Materials
Sep 15, 2002
20
I'm trying to determine the practical thickness limitation of electroless nickel. The base material is 9310 steel. Various literature states that e-nickel can be plated up to .010" thick, however, I am working with a couple of vendors (including a plating house) that states the maximum thickness for E-nickel is approximately .0025". Can anyone provide some input based on actual experience. If plating to a thickness of .005 - .010" is feasible, please provide some hints (i.e., plating chemistry, vendor, etc.) on how it is done.

Thanks
 
Replies continue below

Recommended for you

The practical limit depends upon the size of your wallet.
Are you sure the vendors didn’t say 0.025 inch? Unless the plating solution is old (contains a lot of phosphate by-product,which slows plating and adversely affects the EN deposit properties), this thickness should be attained from most EN solutions in about 3 hours. If the EN is heat-treated for hardness, this should improve adhesion and reduce residual stress if these are concerns.

The Metal Finishing 2003 Guidebook and Directory chapter on Electroless (Autocatalytic) Plating states that electroless nickel (phosphorus type) thickness “generally ranges from 2.5 to 250 um…Deposits… greater than 625 um are currently and successfully being performed. The latter being typical of repair or salvage applications.”

The main problem with thick EN deposits is cost. The chemistry is expensive, solution maintenance must be frequently performed, and it is usually performed at 190oF, so there is a lot of heat and DI water required. Plating rate is usually less than 0.0010”/hr.
Electroplated nickel (from nickel sulfamate solution) is used in electroforming (i.e., very thick deposits). The process can run for hours unattended.

See the link in the thread ‘Residual stress on electroless nicekl plating’
thread338-51904 for MacDermid’s info. Atotech is another good supplier who should be able to tell you which of their EN solutions are low stress/suitable for thick deposits.
although their web site is less helpful: Go to ‘GMF Chemistry,’ then ‘Electroless Nickel.’

See also ‘How to measure the residual stress in electroless nickel plating’
thread332-52658
 
Meant to say 0.0025" in obtained in about 3 hours.
0.025" is an overnight job (which may be why plating shops don't mention).
 