Hello,
I am trying to meet these properties below but for some reason after performing the Heat treatment listed below, I got different results. Part is 6.6" thick. I cannot give anymore than that sorry.
UTS(Ksi)
min: 95
Max 115
Yield(.2 Offset/Ksi)
min: 80
Max: none listed
Elong(2")
Min: 20
max: none listed
RA(%)
min:45
Max: none listed
Hardness
HRC
Min: none listed
Max: 22
HBN
Min: none listed
Max: 237
Heat treatment use:
Normalize: 1650F 4hrs Min. Air cool
Austenitize: 1600F 4hrs Min. Water Quench 10min
Temper: 1225F 7hrs Min. Air cool
Results
TS: 97
Yield: 72
Elong: 25
RA: 71
HBN: 217 Avg, Hi: 229
I am trying to meet these properties below but for some reason after performing the Heat treatment listed below, I got different results. Part is 6.6" thick. I cannot give anymore than that sorry.
UTS(Ksi)
min: 95
Max 115
Yield(.2 Offset/Ksi)
min: 80
Max: none listed
Elong(2")
Min: 20
max: none listed
RA(%)
min:45
Max: none listed
Hardness
HRC
Min: none listed
Max: 22
HBN
Min: none listed
Max: 237
Heat treatment use:
Normalize: 1650F 4hrs Min. Air cool
Austenitize: 1600F 4hrs Min. Water Quench 10min
Temper: 1225F 7hrs Min. Air cool
Results
TS: 97
Yield: 72
Elong: 25
RA: 71
HBN: 217 Avg, Hi: 229