HI

Recently I have encountered a problem in which my carbon steel component is heavily corroded. The component is made up of rolled plates which we recently purchased. I have done XRD analysis of the scale to see if high corrosion rate is due to rolled in scale present on the plates as heavy metal loss was observed. I have got strong peaks of magnetite and low peaks of iron(III) oxide-hydroxide such as Lepidocrocite & Goethite. I have also got halites like sodium, potassium, and Chloride. So this means that the corrosion product mainly formed due to seawater exposure as the item is being transported through sea cargo. Magnetite is usually present in the mill scale so I highly doubt that it is the mill scale presence that has caused high corrosion rate in the presence of seawater. As per my understanding of general rust without mill scale magnetite should not be detected.What you guys think?
 
Replies continue below

Recommended for you

The mill scale is quite adherent while the corrosion product is loose and flaky. It is also huge in mass compared to mill scale.
 
magnetite can also be part of corrosion products and detected without mill scale

metallographic cross section may provide visual evidence of the presence of a mill scale.

water containing dissolved oxygen is very corrosive to carbon steel
 
Did you see pitting or do you have visual evidence of the metal loss?
 
I believe your first assessment (exposure to seawater, and/or salt air) is the correct one - general corrosion with some pitting may be evident.

You accepted this shipment?
 