Low ferrite % for A790UNS S31803 during qualification 3

Status
Not open for further replies.

jazimed

Petroleum
Mar 31, 2015
13
I'm about to prepare a PQR with a Pipe smls NACE BE 4'' S-40S A790UNS S31803 B36.19. Test coupon: two pup pieces of 150mm butt welded each one to another

The welding process used for qualifcation is as follow:

Root Pass:
- GTAW Process
- Filler metal: ER2209 2.4mm
- shield gas: Argon
- Current: 90A
- Voltage: 9 V
- Heat Input 9.7 Kj/cm

Hot Pass:
- SMAW Process
- Filler metal: ER2209-17 2.5mm
- Current: 50-66A
- Voltage: 21-27V
-Interpass temperature: 150°C
- Heat Input 14 Kj/cm

filling Pass:
- SMAW Process
- Filler metal: ER2209-17 2.5mm
- Current: 44-58A
- Voltage: 21-27V
-Interpass temperature: 150°C
- Heat Input 12 Kj/cm

The problem that I'am facing is having a ferrite percentage very low in the Base metal (37%), the HAZ (30%) and the weld joint (25-20%). the mean used for ferrite measurement is the ferritoscope. at the other hand the material certificate of the pipe is indicating 52% of ferrite according to ASTM E562. I don't know whether there is a problem with the base metal or there is something wrong with the welding process. Any help here?
 
Replies continue below

Recommended for you

Just Received the metallography examination report and it's showing the ferrite% as follow: BM= 50%, HAZ= 44%, Weld(root)=34% Weld(cap)=29%. Now I'm 100% sure about the conformity of the base metal.

Obviously, the SMAW process is affecting the ferrite % in the weld. That's why I'm intending to use the GTAW for the hot and filling with the same settings as the root:

Hot and Filling Passes:
- GTAW Process
- Filler metal: ER2209 2.4mm
- shield gas: Argon
- Current: 90A
- Voltage: 9 V
- Heat Input 9.7 Kj/cm
 
Also, shall I keep the interpass temperature 150°C or I have to go below that?
 