Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations SSS148 on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Material Selection Guide

Status
Not open for further replies.

Wasil Ali

Mechanical
May 19, 2022
4
Hello! Good day.

I want to inquire about nozzle pipe and flange material's compatibility with SA-517 Gr. B shell material.

Reference from ASME or any other relevant code would be much appreciated.

Thanks.
 
Replies continue below

Recommended for you

Wasil Ali, refer to ASME SEC II, Part D Table 1A. SA-517 B (plate) is 1/2 Cr-1/5 Mo-V. P 11B, Gr 4 and 115 ksi min tensile.

No exact match in forgings or pipe. Forging SA-182 F2, 1/2 CR-1/2 Mo, P 3 Gr 2, 70 ksi, and pipe SA-335 P2, 1/2 Cr-1/2 MoO, P3, Gr 1, 55 ksi may be usable.

You might be better off to select a different plate like SA-387 2.