Hi all,
I want to ask questions regarding MFI value and degrading of pc/abs.
Virgin PC/ABS's MFI value is 7 and PC/ABS molded part's value is 10. My customer insists on that increasing from 7 to 10 shows that there is a problem with my process and material was decomposed.
In my opinion, MFI testing is not enough by oneself to judge if the material is degraded or not.
Therefore i have it made some testing at the university polymer labaratory.
Performed testings are as follows;
***GPC (Gel Permation Chromatography)
***DSC ( Differential Scanning Calorimetry)
According to the results of these GPC and DSC testings there is no degradation.
I kindly want to ask, if MFI increasing from 7 to 10 absolutely indicates that decomposition has occured?
And MFI testing is enough by oneself for describing the decompositon?
Thank you for your attention..
Best Regards..
I want to ask questions regarding MFI value and degrading of pc/abs.
Virgin PC/ABS's MFI value is 7 and PC/ABS molded part's value is 10. My customer insists on that increasing from 7 to 10 shows that there is a problem with my process and material was decomposed.
In my opinion, MFI testing is not enough by oneself to judge if the material is degraded or not.
Therefore i have it made some testing at the university polymer labaratory.
Performed testings are as follows;
***GPC (Gel Permation Chromatography)
***DSC ( Differential Scanning Calorimetry)
According to the results of these GPC and DSC testings there is no degradation.
I kindly want to ask, if MFI increasing from 7 to 10 absolutely indicates that decomposition has occured?
And MFI testing is enough by oneself for describing the decompositon?
Thank you for your attention..
Best Regards..