Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations IDS on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Modulus of elasticity of steels at high temperaure

Status
Not open for further replies.

asvipin

Mechanical
Nov 27, 2014
36
I want modulus of elasticity of different steels (ss410, 9cr 1mo, 17-4 PH) at high temperature(550C). Anybody please provide some references.

Thanks in advance
 
Replies continue below

Recommended for you

ASME Section II, Part D, Table TM-1. The 17-4 PH will be limited to 480 deg C.
 
Hi,

For the other two materials:

[ul]
[li]AISI 410: corresponding to European X12Cr13 (W.-Nr. 1.4006), YM = 190 GPa @ 400 °C (limiting value for this steel).[/li]
[li]P91: 180 and 167 GPa respectively at 500 and 600 °C for the European equivalent X10CrMoVNb9-1 (W.-Nr. 1.4903).[/li]
[/ul]

All data coming from standard EN 10088-1.
 
From the ASM handbook of High Temperature Property Data
410 at 482C E=158.6GPa (though it isn't smart to take this alloy to this temperature).

Use the ASME Sec II part D tables for the 91.


= = = = = = = = = = = = = = = = = = = =
P.E. Metallurgy, Plymouth Tube
 