I have heard from other code experts the same recommendation as provided by Meteng, but there are some disadvantages to NDT only following PWHT. For P91, if a defect is found following PWHT, one would need to weld repair and PWHT a second time- yet each PWHT increases the aging of the parent material. For alloys as sensitve as P91, NDT before and afer PWHT may be the better approach. If a defect is found prior to the first PWHT, the weld repair would be effectted prior to PWHT and only one PWHT would occur. Also, this method implies the part would need to be cooled to below 100C for NDT, which aids in ensuring complete martensitic transformation prior to PWHT.