I have a set of SA106 steel pipe, which I want to normalize (heat treatment) to improve its properties to reach the minimum values of impact test (Charpy V notched) at -42ºC (-43.6ºF).
I can't get SA333 pipes, so my unique option is to do a normalizing and try to pass the impact test.
The pipes are: 2" XXS, 3" XXS and 6" SCH120.
Can anybode suggest a curve temperature-time to do the normalizing heat treatment (we have equipment for this)?
Would be better to do a 'double' normalizing heat treatment to increase possibilities to pass the impact test?.

Thank you in advance.
Mario


 
Replies continue below

Recommended for you

mariovalenti;
I would try the following using coupons for the normalizing heat treatment followed by impact testing;

1. Heat to 1600-1650 deg F and hold for 1 hr/inch of material thickness.

2. Air cool with air movers.

3. Impact test

4. Repeat steps 1 and 2 above for the second coupon.

By the way, what is your minimum CVN value?
 
The average Cv value is 20J (15 ft-lb)for 10x10 mm specimen.
Thank you very much for your help.
Mario
 
You may not be able to achieve your results. Advise checking the grain size and chemistry. If Al content is above .016% (peferably .020%) fine grain melting practice was employed and your chances will be greater of meeting the requirements. Also check check the sulfur content and carbon & manganese contents. Low carbon and higher Mn contents will also help.

I would also recommend both the single normalizing treatment proposed by metengr and a double normalize treatment on sample coupons.