Pitting corrosion of acylation tank

Status
Not open for further replies.

Larry-MTS

Materials
May 13, 2018
5
A reaction vessel made of SS 316L is subjected to pitting corrosion after 1 year in use. Can anyone help to analyze why the pitting corrosion occurs? Thanks!

Acylation tank: SS 316L
Media: 25% acetic acid, datril, other impurities.
Highest working temp,: 130°C

Please see the pits on internal surface: oh sorry. I can't paste the pic directly to the post

002_p5muvl.jpg


One of our senior engineer says that it probably be caused by the halogen contaminants (especially chlorine ion from potable water).
 
Replies continue below

Recommended for you

ASTM G161 contains a substantial checklist of required information that should be collated and passed to an appropriate organisation for them to draw the most reliable conclusion.

Steve Jones
Corrosion Management Consultant


All answers are personal opinions only and are in no way connected with any employer.
 
Dear Larry-MTS,

Did you find the pits only on the bottom plates? If yes, then can't agree more with your engineer.

Regards.

DHURJATI SEN
 
The grooves are interesting,is that a vertical surface?
In low pH 316 will not handle much Cl.
The curves that I have show pitting at T=130F pH=4 and <10ppm Cl.

= = = = = = = = = = = = = = = = = = = =
P.E. Metallurgy, Plymouth Tube
 