Aug 10, 2005 #1 hockeyb Mechanical Aug 10, 2005 3 US What is a standard thickness tolerance on yellow zinc dichromate plating for fasteners (tread)
Aug 10, 2005 #2 TVP Materials Apr 12, 2002 4,592 US Zinc plating plus yellow chromate is commonly specified as 9 micrometers minimum thickness. It can be as low as 5 micrometers if the corrosion requirement is low or as high as 25 micrometers when greater corrosion resistance is required. Upvote 0 Downvote
Zinc plating plus yellow chromate is commonly specified as 9 micrometers minimum thickness. It can be as low as 5 micrometers if the corrosion requirement is low or as high as 25 micrometers when greater corrosion resistance is required.
Aug 10, 2005 Thread starter #3 hockeyb Mechanical Aug 10, 2005 3 US If 9mm is the standard min. what is the standard max.? I don't want to spec something out of the norm Upvote 0 Downvote
If 9mm is the standard min. what is the standard max.? I don't want to spec something out of the norm
Aug 11, 2005 Thread starter #5 hockeyb Mechanical Aug 10, 2005 3 US Woops, sorry Is there a standard max? Upvote 0 Downvote
Aug 12, 2005 #6 TVP Materials Apr 12, 2002 4,592 US No, there is not a standard maximum. One GM standard limits the maximum to be twice the minimum thickness. Upvote 0 Downvote
No, there is not a standard maximum. One GM standard limits the maximum to be twice the minimum thickness.