The vessel was only partially stress relieved. It was a 60' section that was internally fired through two radial manyways and fully insulated (one near the center of the 60' section, the other near the end). The distortion was in a 40' section between a head and a transition cone. The manyways were fired directly without any deflection or baffles and no inner supports were used (entire vessel was supported on three 24" wide saddles). We questioned this configuration and were assured that it was adequate. There were 19 thermocouples total (only three on each of the firing locations and not directly on the flame impinged locations).
When the firing first began, the vessel 'bananad' (for lack of a better term) from the top portion heating first and it eventually evened out. They then had difficulty getting up to temperature so the upper limit was increased to 1250F to get the coolest point to 1150F min, the whole process took about 52 hrs. The charts did not show a greater than 250F temperature differential between TC, but it also did not show the initial firing (started at around 300-400F).
We of course now realize that they were not experienced enough on a vessel of this size, and we paid for it. We need to find the exact cause and where the scope of responsibility is.
Was the distortion due to the flame impingement (no deflection) or just the prolonged temperature (creep as cb4 pointed out)?
Was the temperture not even and was it higher in areas away from the TC due to thermal pockets?
Was there lack of support under the vessel or would it have still sagged with additional saddles?
To answer your questions unclesyd, The material was SA516 GR70N. There was a distortion of max-min diameter of 4" at the worst spot which was directly where the one of the two firings occured and it was very 'egg shaped' as cb4 asked. The other firing was on the transition cone which was not affected.
As I said, we did manage to fix this successfully, but it was costly (not nearly as much as replacing cans). Any help on this problem would be very much appreciated. Thanks