Rewelding Existing Weld Joints

Status
Not open for further replies.

napster385

Petroleum
Apr 4, 2013
34
Hi Everyone,

When an API 650 tank is dismantled and relocated to a new location, can it be welded on its existing weld joints? Or is it required to cutoff the Heat Affected Zones (approx 2in) on each sides/edges of the plate before rewelding? The API 653 only states that "the existing weld joints shall meet the requirements of the as-built standard."

Appreciate any advise. Thanks.
 
Replies continue below

Recommended for you

The plate containing the previous weld joints should be prepared for welding by use of a new weld prep followed by surface NDT before re-welding.
 
Thank you for your reply metengr.

Does this mean that we don't need to cut off the HAZ area? We will just clean and prepare the plate edges to undergo a new welding process?
 
Yes, if the carbon equivalent (CE) is equal to or less than 0.45 for the plate material, there should be no concern with excessive hardness of the heat affected zones.
 
Ok. Thank you.

Follow up question: What if I weld a high strength steel plate for pressure vessel application? Will there be any special requirements for rewelding? Especially if the plate thickness is over 36mm.
 
I would qualify a WPS with similar plate material where the edges have been welded, the weld has been removed, NDT and re-welded.
 