is there a standard/generic formula/table for calculating stress releif after welding?

thanks in advance
 
Does your question pertain to level or % amount of residual stress remaining or are you referring to stress relief time and temperature data?
 
time & temp data (i.e. ramp, soak & cool down).

thanks
 
To determine time and temperature post weld heat treatment requirements, I would suggest following the post weld heat treatment guidelines outlined in the ASME Boiler and Pressure Vessel Code - Section I for Boilers (Table PW-39) or Section VIII, Div 1 for pressure vessels. The post weld heat treatment requirements associated with the B&PV Code are well established, and are conservative.

You could also use AWS D1.1 Structural Welding Code post weld heat treatment guidelines, as well.

 
thank you
 
Refer to ASME Sec VIII Div 1 UCS 56 for the Time and temperature data for Pressure vessel. UW 40 should give yo somemore useful infor as regards to the modality of PWHT

Further you may refer to ASME/ANSI B 31.3 for the same data for Piping.

Yes there exists a formula which acts as the basis of the Time Temp table. I had it noted down from one of the ASME but don't recollect from where i got it. I think it is in ANSI B 31.3.

Good Luck
 
thanks, i found the charts in ASME B31.1 Table 132 for my application.
 
The formula goes thus


Tp = T*(20+ Log t)/1000000


T = T in Centigrade + 273

t= Hours

For change in PWHT Temperature, how much shoul be the change in soaking time?

Equate Tp and solve to get the soaking time t.



Good Luck
 
I forgot

Tp is the Tempering property
 
bmoorthy,
Please advise me about the reference of the formula. Can we use this formula for all materials?
 
It is not applicable for all material (I am afraid) it ofcourse applicable for CS material. Further you may refer to UCS 56 for the material for which lower temperature and higher soaking is permited. There is a small table given in UCS for tabulating the temperatures and soaking time.


By using this option (Higher soak at lower temp) (if you have not (Welding Engineer) planned) after commencement of fabrication, you may land up in PQR related troubles (Especially if the Vessel is in Sub zero service)

Not discouraging you, but giving you the pit falls. About 4 months back i remember there were discussion on this subject (Supporting PQR).

By proper planning (By welding engineer) this can be amicably settled.

Good Luck

 
Reference Data;

C-Mn Steels (P. No. 1, Gr.1 or 2), Thickness<2”, Initial residual stress = 40,000psi

Remained Residual Stress After PWHT [Reduction Rate]

0 psi [100%] after 2 hours @ 1400 F
1,200 psi [97%] after 1 hour @ 1400 F
3,000 psi [93%] after 4 hours @ 1300 F
3,500 psi [91%] after 2 hours @ 1300 F
4,700 psi [82%] after 1 hour @ 1300 F
3,000 psi [93%] after 16 hours @ 1200 F
4,000 psi [90%] after 12 hours @ 1200 F
5,000 psi [88%] after 8 hours @ 1200 F
5,800 psi [86%] after 4 hours @ 1200 F
6,200 psi [85%] after 2 hours @ 1200 F
7,200 psi [82%] after 1 hour @ 1200 F
7,000 psi [83%] after 8 hours @ 1100 F
7,700 psi [81%] after 4 hours @ 1100 F
8,000 psi [80%] after 2 hours @ 1100 F
9,000 psi [78%] after 1 hour @ 1100 F
8,000 psi [80%] after 8 hours @ 1000 F
9,900 psi [75%] after 4 hours @ 1000 F
10,800 psi [73%] after 2 hours @ 1000 F
12,000 psi [70%] after 1 hour @ 1000 F


Please use this only for reference by lab test

Thomas Eun
 
The formula given by bmoorthy is so called Larson Miller tempering parameter. This is a simple formula for CS only. The draw back is it does not take into account the influence of heating and cooling cycle of the heat treatment. To make a provision for heating and cooling Holloma-Jaffe formula should be used. BTW Centigrade+273°C is Kelvin.
 
The formula given by bmoorthy is so called Larson Miller tempering parameter. This is a simple formula for CS only. The draw back is it does not take into account the influence of heating and cooling cycle of the heat treatment. To make a provision for heating and cooling Holloma-Jaffe formula should be used. BTW Centigrade+273°C is Kelvin.
 
Jaceksan

Can you post the Holloma-Jaffe formula please.
 
Bmoorthy at al

I apologize for letting you wait that long. I didn't see your request earlier. The formula is based on L/M. It is Hollomon and Jaffe formula:


(T+273)*(20+log(te))
HJ = -----------------------
1000


te = th + tc + t


T+273
th = ---------------------
2.3*h*(20-log(h))

T+273
tc = ---------------------
2.3*c*(20-log(c))

Where:
HJ - Hollomon/Jaffe parameter
T - holding temperature [°C]
te - effective holding time [h]
th - correction in holding time for heating cycle [h]
tc - correction in holding time for cooling cycle [h]
h - heating rate [°C/h]
c - cooling rate [°C/h]

The formula was derived empirically and it seems to reflect better the effects of heating and cooling on tempering degree of metal than LM parameter. I used this formula to asess the remaining life of pressure vessels after multiple PWHT cycles. It was also used to set the parameters of PWHT simulation cycles.

Regards