Hello,
A colleague yesterday regaled me with stories of "tin whiskers" (presumably strands of tin escaping) occurring in a vacuum when the wrong stainless is used. But he couldn't remember which stainless is the "wrong" one. I have never heard of this.
1. Is there any truth to the "tin whiskers" story?
2. If so, with what stainless does this occur?

Thanks,
'ziner

Peace Through Superior Fire-Power!
 
Replies continue below

Recommended for you

There was a show tonight on the History Channel that discussed various Engineering Disasters. There was quite a discussion specifically about Tin Whiskers and the failures of electronic equipment. There was quite a few of SEM pictures of the whiskers. There is a lot of work being done at the University of Maryland.
 
Nothing to do with stainless steel.
Vacuum isn't necessary, either.

Tin whiskers nucleate & grow from the surface of ~pure tin electroplating. Alloying can prevent, but unfortunately, lead was one of the most effective whisker inhibitors.
Some whiskers from the NASA Goddard Center:

TMW05_09CTR_wiskshapes_420px.jpg


Besides the afore-mentioned sites, the electronics industry has published some useful documents on mitigating the problem:
Current Tin Whiskers Theory and Mitigation Practices Guideline - JP002 (March 2006):

iNEMI Recommendations on Lead-Free Finishes for Components Used in High-Reliability Products Version 4 (12-1-06)
An article "Tackling tin whisker test" gives conditions for accelerating possible whisker growth from samples:

NIST has also done some work as part of their lead-free solders program:
"The Formation of Whiskers on Electroplated Tin Containing Copper"
Although a common belief that tin whiskers never form from galvanizing (hot dipped zinc coating on steel), cases have been found:
"The Driving Force Behind Whisker Growth"
 