Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations KootK on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

TSA AISI316L against 22 Cr duplex 1

Status
Not open for further replies.

MaxNeg63

Petroleum
Jul 6, 2005
23
Hello everybody. Is there anybody who has any knowledge about the use of thermally sprayed alluminium coated AISI316L against bare 22 Cr duplex steel within an environment containing hydrocarbon and water?
thanks a lot
Max
 
Replies continue below

Recommended for you

It wouldn't be considered normal practice (by me anyway) to resort to applying thermal spray aluminium to a CRA material. It's horses for courses and if you have to adopt TSA then you have backed the wrong horse. What corrosion mechanism are you trying to protect against?

Steve Jones
Materials & Corrosion Engineer
 
Thanks Steve. Supplier is proposing such solution to protect 316L against SCC at temperatures higher than 50 °C.
My doubts regard the inherent porosity of thermal spray coatings and therefore the contact between substrate material and aggressive environment.
 