Dear all,
i had etched a piece of annealed stainless steel 440C material with 10% Oxalic acid, however I can't identify any traces of martensitic structure. In addition, are the white islands carbide?

I had attached a photomicrograph taken at 500X for viewing.

Thanks!
 
Replies continue below

Recommended for you

How are you expecting martensitic structure in an annealed condition? martensitic structure is a quenched annealed structure for as I know.
 
The annealed 440C microstructure consists of round globules, which are carbides, in a ferrite matrix. This is typical for fully annealed material. There should be no martensitic structure.
 
Typically annealed microstructure. Why were you expecting any martensite in them?

_____________________________________
"It's better to die standing than live your whole life on the knees" by Peter Mayle in his book A Good Year
 
Status
Not open for further replies.

Part and Inventory Search

Sponsor