We have a part fabricted from 7075-T652 aluminum and subjected to axial compression loading and bending in two orthogonal planes. We have problems with fatigue failures and have performed an FEA to address high-stress areas and reduce stress concntrations. Currently, the maximum applied stresses are ar or below 20 kpsi in most areas. The part has passed a 3 million cycle fatigue test in the unanodized condition. After a hard-coat anodize layer (0.0004" thick) is applied, the part fails at about 380,000 cycles. The failure is at the tangent point of a radius between section changes. The FEA shows the Max Principal Tensile Stress magnitude is approximately 20 - 26 kpsi in the area of the failure. (A fatigue limit of about 36 kpsi was assumed for the material). Any ideas concerning a possible reason for the huge change in performance is welcome.
 
Replies continue below

Recommended for you

The hardcoat anodizing is the cause of the huge reduction in fatigue performance. It is well-known that hard ceramic layers like anodizing on aluminum initiate cracks and reduce fatigue life.
 
Reduction in fatigue life of anodized aluminium is a well-recognized phenomenon with a plethora of information available.

For example, according to MIL-A-8625F ANODIC COATINGS FOR ALUMINUM AND ALUMINUM ALLOYS,

6.10.7 Effect on fatigue. The fatigue properties of aluminum alloys can be severly reduced by anodic coatings.

Regards,

Cory

Please see FAQ731-376 for tips on how to make the best use of Eng-Tips Fora.
 
The alternative, if the hardness of the anodizing is not a design requirement, is to use chromate conversion coating, (Mil-C-5541E), one commercial version of it is called allodine.

 
You can also shot peen prior to the anodize to gain a little fatigue resistance. Another improvement can be done by specifying a smoother surface.

What kt are you getting from the fem?
 