8620H Temper Depth

Status
Not open for further replies.

tmoney99

Mechanical
Oct 20, 2010
2
I have a part, 8620H, with an M20x1.5 OD thread on it. The part is to be machined and then quenched to 980MPA. It states the thread must not be hardened.

This isnt really a case depth type thing, I thought quenching was a metallurgical transformation (martensite?). Is there a level at which the hardening decreases?

Does anyone have experience with this type of situation?

The cross section is R20mm (.79) and about the same in length.

Thanks,
Tyler.
 
Replies continue below

Recommended for you

The material and the stated requirements are in conflict. The stated mechanical property requirement of 980 MPa is roughly comparable to a grade 10.8 metric fastener and you can't get there without a fully hardened, quenched and tempered product. You also can't get there with SAE 8620H steel. The only time I have seen a requirement for non hardened threads on a heat treated product is a product that is induction hardened, with the threads left soft, i.e. something like a ball stud.
 
My apologies, this thread can be closed.

I assumed to much while reading the drawing.....Getting ahead of myself.

Thanks uncle and swall.
 
FYI only.

This is a low carbon cast iron/steel. normally, the surface is carburized for higher hardness and wearing resistance. Then quenched and tempered. It does not make a sense to do the inductive hardening w/o carburizing.
 
Another option is to carburize the part followed by induction annealing of the thread section.
 