Does anybody have a good information (probably a link) about the convenience or real effects in the use of Dehydrogenation Heat Treatment (DHT) after welding for welds in P4 and P5 materials?
 
Replies continue below

Recommended for you

What do you need to know exactly? For piping and pressure vessels, hydrogen back-out or a post weld bake is normally performed, immediately after welding is completed, at 500 deg F minimum for 1 hour per inch of nominal weld deposit thickness. This technique is not necessary IF low hydrogen electrodes were used in fabrication/repair.
 
Thanks first of all. We are a pressure vessels manufacturer and we have welded for many years reactors and others made of Cr-Mo materials, mainly P4. The way we apply the DHT treatment often depends on the client`s requirements but we do not have any clear criteria to propose in the case that no requirements exist. Also, there is no too much information about this issue, I mean, about the real effects ( difussible hydrogen decreasing, toughness improvement, etc..) of applying different DHT's. It would be great to find any good information ( probably some complete technical article) as a basis to define the need for DHT for different thicknesses, welding conditions ( for example high restrained welds) based in knowing the real effect of the DHT.

Thanks in advance
 
Ok. I believe what you refer to as your DHT is actually post weld heat treatment (PWHT) in accordance with Code requirements, is this correct?

If so, when you respond back, I can provide some guidance on this matter for these materials.
 