Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations cowski on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Magnetic properties of SS 416 (B-H)

Status
Not open for further replies.

bgilbert

Mechanical
Feb 4, 2005
14
Anyone knows where I can find the B-H curve of the SS 416 ?
Thanks!
 
Replies continue below

Recommended for you

Look for one on 410. It will be important to match your same heat treat condition. (Q&T? what temper temperature?)

= = = = = = = = = = = = = = = = = = = =
Plymouth Tube
 
OK, I'll try to find the Q&T, but in the mean time, do you have information about the 410 or 416? Where should I look?
Thanks
 
I have this data that I downloaded when I tried using FEMM.
I make no claims to it's accuracy.

B (T) H (A/m)
0.000 0.0
0.200 318.3
0.426 477.5
0.761 795.8
1.097 1591.6
1.233 2387.3
1.335 3978.9
1.460 7957.8
1.590 15915.5
1.690 31831.0
1.724 44456.3
1.740 55704.3
 