Arulkumar P
Electrical
- Jun 15, 2012
- 11
One of my client specification is asking "CS & LTCS ( Boiler Quality) plate above 50 mm is required through thickness test as per SA 770 shall be conducted and minimum reduction in area of 35% shall be ensured."
Clause 5 of acceptable standard SA 770 in ASME Sec IIA part A code shows "test shall have a minimum reduction of area no less than 20 %."
Clause 3.9 of Sec VIII Div 2 shows "For carbon and low alloy steels, the reduction of area shall not be less than 30%"
My query is
1 what is the background of the CS & LTCS (BQ) Plate through thickness test percentage reduction area minimum 20%,30%&35% or higher?
2.what is the high alloy materiel( i.e.-Stainless steel and nickel alloy steel)through thickness test percentage?
Clause 5 of acceptable standard SA 770 in ASME Sec IIA part A code shows "test shall have a minimum reduction of area no less than 20 %."
Clause 3.9 of Sec VIII Div 2 shows "For carbon and low alloy steels, the reduction of area shall not be less than 30%"
My query is
1 what is the background of the CS & LTCS (BQ) Plate through thickness test percentage reduction area minimum 20%,30%&35% or higher?
2.what is the high alloy materiel( i.e.-Stainless steel and nickel alloy steel)through thickness test percentage?