Hi,
I am wondering how to work out the thermal expansion calc of a ring with OD 1000mm and ID 800mm and L20mm. I
I am heat treating a nickel alloy ring at 1000°C and I am wondering how much the ring will grow at the OD, ID and L at this temperature. I am only looking for a rough estimation.
The linear thermal expansion from 20-1000°C of the alloy is 18.2 X 10-6.
Also, if I was to heat treat another ring with an OD 1000mm but with a bore of 300mm and L50 would the rate of expansion be the same. ie would the OD in both rings end up the same size at 1000°C?
I am wondering how to work out the thermal expansion calc of a ring with OD 1000mm and ID 800mm and L20mm. I
I am heat treating a nickel alloy ring at 1000°C and I am wondering how much the ring will grow at the OD, ID and L at this temperature. I am only looking for a rough estimation.
The linear thermal expansion from 20-1000°C of the alloy is 18.2 X 10-6.
Also, if I was to heat treat another ring with an OD 1000mm but with a bore of 300mm and L50 would the rate of expansion be the same. ie would the OD in both rings end up the same size at 1000°C?