How long should concrete spread foundations cure before they are backfilled?
 
Replies continue below

Recommended for you

Depends on a lot.....temperature, humidity, curing process, construction sequencing, steel erection, etc.

I would say a minimum of 3 days with good cylinder breaks, but otherwise 7 days or until 75% of f'c is obtained.

 
Assuming 30mpa concrete and normal compaction equipment, 3 days should give you about 15mpa strength. Plenty of capacity. Ask for 3 day cylinder results before compaction.
 