In AMS 2774, does anyone know what the metallurgical reason for the higher annealing temperature at 2050 F temperature for alloy 625 if brazing will follow? Normally, annealing would be at 1900 F, but footnote 9 in rev G requires a 2050 F anneal if high-temperature brazing is to follow.
 
Replies continue below

Recommended for you

If you anneal 625 below 1900F you do not dissolve the stabilizers.
With high temp brazing the temps are often 1900-2100.
And they want you to solution anneal prior to the braze so that you don't use the braze cycle as your anneal and end up with non-uniform results.
Get the correct microstructure first, then braze.

= = = = = = = = = = = = = = = = = = = =